| Titanium β-alloy Ti-10V-2Fe-3Al | ||||
| Chemical composition: O=0.13% max., V=10%, Fe=2%, Al=3%, Ti balance | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 4.65*10³ | kg/m³ | 290 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 103 | GPa | 15000 | ksi |
| Thermal expansion (20 ºC) | 9.7*10-6 | ºCˉ¹ | 5.4*10-6 | in/(in* ºF) |
| Tensile strength | 1310 | MPa | 190000 | psi |
| Yield strength | 1228 | MPa | 178000 | psi |
| Hardness | 41 | HRC | 41 | HRC |
| Solution temperature | 760 | ºC | 1400 | ºF |
| Aging temperature | 500 | ºC | 930 | ºF |
| Aging time | 8 | hrs. | 8 | hrs. |
| Melting temperature | 1649 | ºC | 3000 | ºF |
| Beta Transus temperature | 796 | ºC | 1465 | ºF |