| Spinodal Bronze ToughMet3 CX | ||||
| Chemical composition: Ni=15.0%, Sn=8.0%, Cu=balance | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.94*10³ | kg/m³ | 558 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 128 | GPa | 18500 | ksi |
| Thermal expansion (20 ºC) | 16.4*10-6 | ºCˉ¹ | 9.1*10-6 | in/(in* ºF) |
| Specific heat capacity | 377 | J/(kg*K) | 0.09 | BTU/(lb*ºF) |
| Thermal conductivity | 38.1 | W/(m*K) | 264 | BTU*in/(hr*ft²*ºF) |
| Thermal diffusivity | 0.9*10-5 | W/(m*K) | 0.014 | in²/s |
| Tensile strength (cast and spinodally hardened) | 735 | MPa | 105000 | psi |
| Yield strength (cast and spinodally hardened) | 690 | MPa | 100000 | psi |
| Elongation (cast and spinodally hardened) | 5 | % | 5 | % |
| Hardness (cast and spinodally hardened) | 28.5 | RC | 28.5 | RC |