to Metals
to Coating technologies
Dr. Dmitri Kopeliovich
Rinsing is a preparation of a work part for a subsequent operation by a dilution of the chemical substances adhered to the part in the previous operation.
An improperly rinsed part may produce stains on the surface and cause an insufficient adhesion strength of the subsequent coating.
In addition, poor rinsing results in a contamination of the subsequent tanks.
Effectiveness of rinsing is measured by the parameters called Dilution Factor.
Dilution Factor (D) is the ratio of the concentration of the main chemical in the process tank to the rise of its concentation in the rinse tank as a result of the rinsing step.
Dilution Factor may also be calculated as the ratio of the rinsing tank volume Vr to the drag-in volume Vd:
D = Vr/Vd (1)
A combination of a low concentration of the main chemical substance in the rinse tank with a low rinsing water flow may be achieved by the following rinsing methods:
According to the formula (1) good rinsing may be achieved by means of a large amount of water flowing at a rate exceeding the the drag-in rate by the factor D (Dilution Factor).
However the amount of rinse water may be considerably reduced in the rinsing practice called Countercurrent Rinsing.
Countercurrent rinsing is the rinsing operation conducted in a sequence of rinsing tanks through which water flows in the diraction opposite to the direction of the work part.

Fresh water enters the last (cleanest) rinsing tank at its bottom, crosses the tank space and leaves the tank by overflow on the top. The water stream flows down driven by gravity to the bottom where it enters the preceding tank. The process goes and water exit the rinsing system in the first (dirtiest) tank.
Commonly countercurrent rinsing systems have a sequence of either two or three rinsing tanks (two-stage countercurrent rinsing, three-stage countercurrent rinsing).
Countercurrent rinsing allows drustical reduction of rinsing water (by 90-95%).
In a three-stage countercurrent rinsing system with the Dilution Factor D=20 the chemical concentration in the last rinse tank is:
Cr = Cd/203 = Cd/800
Where Cd/ is the concentration of the chemical in the drag-in (in the previous operation tank).
Rinsing water flow F necessary to dilute (rinse) the dag-in from the concentration Cd to the concentration Cr in a countercurrent rinsing with N stages may be calculated as follows:
F = N*Fd*(Cd/Cr)1/N
Where Fd is the drag-in flow rate.
In the example of Cd/Cr = 1000 we obtain:
F/Fd (one tank) = 1000
F/Fd (two tanks) = 63
F/Fd (three tanks) = 30
Thus three-stage countercurrent rinsing allows reduction of the rinsing water flow by the factor 33 (as compared to a simple rinsing).
to top
Static rinse tank is used in order to reduce drag-out from a process tank. The work part is submerged into the static rinse tank twice: just before going to the process tank (pre-dip) and as a first rinsing step after the part came out of the process tank.
After some time the concentrations of the chemicals in the static tank stabilize at the level of 50% of those in the process tank.
Therefore static rinse tank allows on one hand to reduce drag-in enetring the countercurrent rinsing system and on the other hand to reduce the drag-out from the process tank to a half. In addition, the solution from the rinse tank may be periodically added to the process tank to compenstae water evaporated from it and to recover some of the draged-out chemicals.
to top
Agitation (movement) of rinsing water enhances dissolution of the chemicals adhered to the work part surface. Therefore agitation increases rinsing efficiency and allows reduction of the rinsing time.
The following agiation techiques are used:
Spray rinsing is a rinsing technique utilizing the effect of water jets spraying over the work part by nozzles installed at the tank top.
Spray rinsing may be used two configurations:
Spray rinsing over a rinsing tank results in a reduction of water consumption by 25% as compared to dip rinsing.
Spray rinsing is commonly combined with a dip rinsing.
Air knives are jets of pressurized air blowing the liquid (drag-out) adhered to the work part off when the jig is beeing withdrawn from the process tank up.
Air knives are produced by nozzles installed at the tank top.
Air knives are capable to reduce drag-out by 75%. The drag-out blown off from the work part is returned back to the tank. Use of air knives allows considerable reduction of the rinsing water consumption.
The main disadvantage of air knives is oxidation (staining) of the work part surface by the pressurized air.
to top
Reactive rinsing utilizes the effect of neutralization of alkaline solution dragged from the Alkaline cleaning bath by the acid contained in the rinsing tank.
Commonly the Surface preparation prior to Electroplating includes Alkaline cleaning, rinsing, acid activation and rinsing after acid treatment.
If rinsing operations are performed in the same rinsing tank the alkaline drag-out is mixed with the acidic drag-out and neutralize each other.
The reactive rinsing method considerably reduces drag-in of alkaline solution into the acid process tank.
to top
to Metals