Dr. Dmitri Kopeliovich
Salt bath heat treatment is a heat treatment process comprising an immersion of the treated part into a molten salt (or salts mixture).
| No. | Composition | Approximate melting poing | Work temperature range |
|---|---|---|---|
| 1 | NaOH 75% KOH 19% H2O 6% | 284ºF (140ºC) | 320-752ºF (160-280ºC) |
| 2 | KOH 50-60%% NaOH 50-40% | - | 572-752ºF (300-400ºC) |
| 3 | KNO3 100% | 639ºF (337ºC) | 662-930ºF (350-500ºC) |
| 4 | KNO3 50-60% NaNO2 50-40% | 275ºF (135ºC) | 320-1022ºF (160-550ºC) |
| 5 | NaNO3 50-60% NaNO2 50-40% | 293ºF (145ºC) | 311-932ºF (150-500ºC) |
| 6 | KNO3 50-60% NaNO3 50-40% | 437ºF (225ºC) | 500-1112ºF (260-600ºC) |
| 7 | NaNO3 100% | 698ºF (370ºC) | 752-1110ºF (400-600ºC) |
| 8 | NaCl 10-15% KCl 20-30% BaCl2 40-50% CaCl2 15-20% | 752ºF (400ºC) | 932-1472ºF (500-800ºC) |
| 9 | NaCO3 45-55% KCl 55-45% | 842ºF (450ºC) | 1022-1652ºF (550-900ºC) |
| 10 | BaCl2 50% KCl2 30% NaCl 20% | 1004ºF (540ºC) | 1058-1652ºF (570-900ºC) |
| 11 | BaCl2 70-96% NaCl 30-4% | 1112-1472ºF (600-800ºC) | 1292-2282ºF (700-1250ºC) |