Cast copper alloy C83600 (Ounce Metal)
Chemical composition: Zn=5%, Pb=5%, Sn=5%, Cu=85%
Property Value in metric unit Value in US unit
Density 8.83 *10³ kg/m³ 551 lb/ft³
Modulus of elasticity 93.1 GPa 13500 ksi
Thermal expansion (20 ºC) 18.0*10-6 ºCˉ¹ 10.0*10-6 in/(in* ºF)
Specific heat capacity 377 J/(kg*K) 0.090 BTU/(lb*ºF)
Thermal conductivity 72 W/(m*K) 499 BTU*in/(hr*ft²*ºF)
Electric resistivity 11.5*10-8 Ohm*m 11.5*10-6 Ohm*cm
Tensile strength (sand cast) 255 MPa 37000 psi
Yield strength (sand cast) 117 MPa 17000 psi
Elongation (sand cast) 30 % 30 %
Fatigue strength (sand cast) 76 MPa 11000 psi
Hardness (sand cast) 60 HB(500) 60 HB(500)
Liquidus temperature 1010 ºC 1850 ºF
Solidus temperature 854 ºC 1570 ºF