Cast copper alloy C95600 (Aluminum Bronze)

(submitted by the website administration)

Cast copper alloy C95600 (Aluminum Bronze)
Chemical composition: Al=7.0%, Si=2.5%, Cu=91.5%
Property Value in metric unit Value in US unit
Density 7.70 *10³ kg/m³ 481 lb/ft³
Modulus of elasticity 103 GPa 15000 ksi
Thermal expansion (20 ºC) 16.6*10-6 ºCˉ¹ 9.2*10-6 in/(in* ºF)
Specific heat capacity 419 J/(kg*K) 0.10 BTU/(lb*ºF)
Thermal conductivity 38.6 W/(m*K) 268 BTU*in/(hr*ft²*ºF)
Electric resistivity 20.4*10-8 Ohm*m 20.4*10-6 Ohm*cm
Tensile strength (sand cast) 517 MPa 75000 psi
Yield strength (sand cast) 234 MPa 34000 psi
Elongation (sand cast) 18 % 18 %
Hardness (sand cast) 140 HB(3000) 140 HB(3000)
Liquidus temperature 1004 ºC 1840 ºF
Solidus temperature 982 ºC 1800 ºF