| SAE 1090 | ||||
| Chemical composition: C=0.90%, Mn=0.75%, P=0.04% max, S=0.05% max | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 202 | GPa | 29300 | ksi |
| Thermal expansion (20 ºC) | 11.5*10-6 | ºCˉ¹ | 6.39*10-6 | in/(in* ºF) |
| Specific heat capacity | 473 | J/(kg*K) | 0.113 | BTU/(lb*ºF) |
| Thermal conductivity | 49.8 | W/(m*K) | 345 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 1.74*10-7 | Ohm*m | 1.74*10-5 | Ohm*cm |
| Tensile strength(cold drawn and annealed) | 696 | MPa | 101000 | psi |
| Yield strength(cold drawn and annealed) | 540 | MPa | 78300 | psi |
| Elongation(cold drawn and annealed) | 10 | % | 10 | % |
| Hardness(cold drawn and annealed) | 92 | RB | 92 | RB |
| Tensile strength (hot rolled) | 841 | MPa | 122000 | psi |
| Yield strength (hot rolled) | 460 | MPa | 66700 | psi |
| Elongation (hot rolled) | 10 | % | 10 | % |
| Hardness (hot rolled) | 98 | RB | 98 | RB |