SAE 1030 | ||||
Chemical composition: C=0.30%, Mn=0.75%, P=0.04% max, S=0.05% max | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 200 | GPa | 29000 | ksi |
Thermal expansion (20 ºC) | 11.7*10-6 | ºCˉ¹ | 6.5*10-6 | in/(in* ºF) |
Specific heat capacity | 486 | J/(kg*K) | 0.116 | BTU/(lb*ºF) |
Thermal conductivity | 48.7 | W/(m*K) | 338 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 1.66*10-7 | Ohm*m | 1.66*10-5 | Ohm*cm |
Tensile strength (hot rolled) | 470 | MPa | 68200 | psi |
Yield strength (hot rolled) | 260 | MPa | 37700 | psi |
Elongation (hot rolled) | 20 | % | 20 | % |
Hardness (hot rolled) | 75 | RB | 75 | RB |
Tensile strength (cold drawn) | 525 | MPa | 76100 | psi |
Yield strength (cold drawn) | 440 | MPa | 63800 | psi |
Elongation (cold drawn) | 12 | % | 12 | % |
Hardness (cold drawn) | 80 | RB | 80 | RB |