SAE 1117 (free cutting) | ||||
Chemical composition: C=0.17%, Mn=1.20%, P=0.04% max, S=0.08%-0.13% | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 200 | GPa | 29000 | ksi |
Thermal expansion (20 ºC) | 11.5*10-6 | ºCˉ¹ | 6.39*10-6 | in/(in* ºF) |
Specific heat capacity | 481 | J/(kg*K) | 0.115 | BTU/(lb*ºF) |
Thermal conductivity | 51.2 | W/(m*K) | 355 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 1.74*10-7 | Ohm*m | 1.74*10-5 | Ohm*cm |
Tensile strength (hot rolled) | 400 | MPa | 58000 | psi |
Yield strength (hot rolled) | 220 | MPa | 31900 | psi |
Elongation (hot rolled) | 25 | % | 25 | % |
Hardness (hot rolled) | 66 | RB | 66 | RB |
Tensile strength (cold drawn) | 475 | MPa | 68900 | psi |
Yield strength (cold drawn) | 400 | MPa | 58000 | psi |
Elongation (cold drawn) | 12 | % | 12 | % |
Hardness (cold drawn) | 86 | RB | 86 | RB |